| Ferritic Stainless Steel Alloy Chemistry | ||||||||||||
| Carbon Max |
Manganese Max |
Silicon Max |
Chromium Min-Max |
Nickel Max |
Molybdenum Max |
Phosphorous Max | Sulfur Max |
Copper Max |
Iron | Other | Melting Range |
|
|---|---|---|---|---|---|---|---|---|---|---|---|---|
| Alloy Type | ||||||||||||
| 409/Nb Investment Cast | 0.16 | 1.5 | 2.0 | 10.5-11.75 | 0.50 | 0.045 | 0.045 | Bal. | Cb (Nb) 8*C Min 1.00 Max | 2550-2650 | ||
| 442 (CB-30) Investment Cast | 0.30 | 1.00 | 1.50 | 18.0-22.0 | 2.0 | 0.04 | 0.04 | Bal. | 2650-2750 | |||
| 446 (CC-50) Investment Cast | 0.50 | 1.00 | 1.50 | 26.0-30.0 | 4.0 | 0.04 | 0.04 | Bal. | 2650-2750 | |||
| Ferritic Stainless Steel Alloy Properties | |||||||
| Condition | Tensile Strength | 0.2% Yield Strength | % Elongation Range (2.5 cm or 1”) | Hardness Max | |||
|---|---|---|---|---|---|---|---|
| Alloy Type | English PSI | Metric MPa | English PSI | Metric MPa | |||
| 409/Nb Investment Cast | Annealed | - | - | - | - | - | 100 Rb |
| 442 (CB-30) Investment Cast | Annealed | 65-100,000 | 448-689 | 30-70.000 | 207-483 | 15-25 | 241 BHN Max |
| 446 (CC-50) Investment cast | Annealed | 55-95,000 | 379-655 | - | - | - | 241 BHN Max |
Mechanical Property values are for
information only. They are determined from test bars and do not necessarily
apply to castings. Any requirements for mechanical properties that are beyond the
above information must be discussed with and agreed to by WPCC.
| Ferritic Stainless Steel Alloy Cross-Index | ||
| Alloy or Type | AMS | Other Designation |
|---|---|---|
| 409/Nb Investment Cast | ||
| 442 (CB-30) Investment Cast | ASTM A743 CB-30 | |
| 446 (CC-50) Investment cast | ASTM A743 CC-50 | |